SINT-A50 is a low-density tin bronze sintered bearing material per DIN 30910-3. Standard material (preferred grade). High porosity provides maximum oil retention for self-lubricating bearing applications.
| Element | Content |
|---|---|
| Cu | Rest (Balance) |
| Sn | 9–11% |
| C | < 0.2% |
| Other | < 2% |
| Property | Value |
|---|---|
| Density | 6.4–6.8 g/cm³ |
| Porosity | 25 ± 2.5% |
| Radial Crushing Strength K | > 120 N/mm² |
| Hardness HB | > 25 |
| Thermal Conductivity | 27 W/mK |
Comparable Standards: MPIF CT-100-K17 / ISO 5755 P4011Z. Radial crushing strength K is measured on calibrated bearings Ø 10/16 × 10. Oil content is minimum 90% of open porosity.
|
Standard |
Material Code |
Density (g/cm3) |
Hardness |
Tensile Strength |
Compositions (%) |
||||||||
|
Ultimate (MPa) |
Yield (MPa) |
Fe |
Cu |
C |
Ni |
Mo |
Mn |
Cr |
Sn |
||||
|
DIN 30910-4:2004-05 |
Sint-A50 |
6.4-6.8 |
>HB25 |
140 |
100 |
|
Bal. |
<0.2 |
|
|
|
|
9-11 |